WELDER 01
WELDER QUALIFICATION Nº 01 (RANGE QUALIFIED):
P NUMBER: P1 À P11, P34, P41 À 47
Ø PIPE: ? 1"
F NUMBER: 6
-----------------------------------------------------------

SITUATION
P NUMBER: 10H (DUPLEX)
Ø PIPE: 1"
F NUMBER: N.A. (THE FILLER METAL HAS NOT F NUMBER)
-----------------------------------------------------------

DOES WELDER 01 QUALIFIED FOR THIS SITUATION, ACCORD ASME IX?


 
Base material and OD size are compliant. What is the weld deposit thickness range? This is also an essential welding variable. Please review ASME Section IX.
 
F No. is an essential variable for welder qualification. Review QW-404.15 and QW-354 thru Qw-357.

 
I know F number is an essential variable like another variables that I didn't mention.
I just wanna know if the welder qualified F number 6 can weld a filler metal without F number, assuming that the other variables it´s correct.
And if possible, where I find this in ASME?

Thanks the attention




 
Claytonsilva;
No, a welder currently qualified to weld with F-No 6 cannot weld using an unidentified filler metal, review ASME Section IX, QW-350 (these list the essential variables for welder performance qualification, and F-No change for filler metal is an essential welding variable for performance qualification, as mentioned above).

A welder could weld with any unidentified F-no weld rod (even coat hanger wire) provided the welder either qualified a weld procedure specification for using this filler metal or has run a coupon to qualify for this specific filler metal composition using a WPS that was qualified for this filler metal composition.
 
Metengr,
About this situation,
QW-356 (GTAW) - Essential Variables

QW-404.15 Change of F-number
QW-404.15 A change from one F-Number in table QW-432 to any other F-Number or to any other filler metal, except as permitted in QW-433

I understood, the F-number has changed, F-number 6 to unidentified filler metal, but ASME doen´t explain about unidentified filler metal or does?
 
It does, really. An F-No 6 filler metal qualification cannot be used on a filler metal that does not have an F-No or does not belong to an AWS Specification. All you need to do is to qualify a weld procedure with this unique filler metal and the welder will be qualified to weld with this filler metal for your project. For other welders, they can run a coupon using this WPS and they are qualified for using this filler metal.
 