stuus
Civil/Environmental
- Sep 28, 2004
- 7
Hello all,
I am in charge of a paving project using standard 1/2" PG-64-10 Caltrans AC mix. The latest area was paved a couple hours before a rain event. This area is now uniformly covered with small puddles of water that doesn't drain off. The grades are around 1% and other areas of the project shows water draining off.
The only theory I have is that the oils from the curing, freshly paved asphalt mixed with the water and therefore it doesn't drain off.
Has anyone had similar experiences? Could I be correct regarding the oil or is there some other explanation?
Thanks,
I am in charge of a paving project using standard 1/2" PG-64-10 Caltrans AC mix. The latest area was paved a couple hours before a rain event. This area is now uniformly covered with small puddles of water that doesn't drain off. The grades are around 1% and other areas of the project shows water draining off.
The only theory I have is that the oils from the curing, freshly paved asphalt mixed with the water and therefore it doesn't drain off.
Has anyone had similar experiences? Could I be correct regarding the oil or is there some other explanation?
Thanks,