ESDU MMDH lists the following Euro, French and German equivalents, just in case they're more readily available:
FE-PL2110
AIR9160 16 NCD 17
1.6723
In addition S156 and German spec 1.6722 seem to be a VAR version of almost the same material (a fraction less Si and tighter control of harmful impurities, see below), which may also be included in the above Euro and French specs.
Also just in case, S82 is aka prEN2767 (bar) and prEN2768 (forging).
There are no US specs listed and it doesn't have a common name.
S82 has the following composition:
Element Min % Max %
C 0.14 0.18
Si 0.15 0.4
Mn 0.25 0.55
Cr 1 1.4
Mo 0.2 0.3
Ni 3.8 4.3
P — 0.025
S — 0.020
S156 has the following composition:
Element Min % Max %
C 0.14 0.18
Si 0.1 0.35
Mn 0.25 0.55
Cr 1 1.4
Mo 0.2 0.3
Ni 3.8 4.3
P — 0.015
S — 0.012
However, I reckon TVP has the right of it in terms of a way forward for you.