Good morning,
We have one U-Tube Heat Exchanger where the tubes made of SS (SA 789) and others like baffles, tie rods shell and caps are made of CS (ASTM 516 Gr. 60).
First, what is the purpose of using the two dissimilar metals for the design?
Secondly, and because of this design the baffles and tie rods were heavily attacked by galvanic corrosion after years of operation, their replacement is deemed necessary now.
Saying that, and in order to insert the new baffles and tie rods to the good condition tubes, I propose to cut the tubes slightly before the tube sheet. So, is that practically acceptable? and what effects on the process and heat transfer efficiency after shortening the tubes by few centimetres?
Cooler details:
Design pressure: Shell 38 bar and Tubes 55.5 bar
Design temperature: Shell 70 degrees Celsius and tubes 170 degrees Celsius
Fluid: Shell Cooling Water and tubes HC+H2O
No. of passes: 1 for the shell and 2 for the tubes.
Capacity: Shell 430 liters and tubes 150 litres
Tubes: Diameter 19.05 X 1.65 - 6096 long.
Best regards,
We have one U-Tube Heat Exchanger where the tubes made of SS (SA 789) and others like baffles, tie rods shell and caps are made of CS (ASTM 516 Gr. 60).
First, what is the purpose of using the two dissimilar metals for the design?
Secondly, and because of this design the baffles and tie rods were heavily attacked by galvanic corrosion after years of operation, their replacement is deemed necessary now.
Saying that, and in order to insert the new baffles and tie rods to the good condition tubes, I propose to cut the tubes slightly before the tube sheet. So, is that practically acceptable? and what effects on the process and heat transfer efficiency after shortening the tubes by few centimetres?
Cooler details:
Design pressure: Shell 38 bar and Tubes 55.5 bar
Design temperature: Shell 70 degrees Celsius and tubes 170 degrees Celsius
Fluid: Shell Cooling Water and tubes HC+H2O
No. of passes: 1 for the shell and 2 for the tubes.
Capacity: Shell 430 liters and tubes 150 litres
Tubes: Diameter 19.05 X 1.65 - 6096 long.
Best regards,