Nov 16, 2004 #1 RogerF Mechanical Joined Oct 7, 2002 Messages 11 Location NO HI! I have a small question that I hope someone can help me answer. I want to connect an flow-element made of Hastalloy C22 into a Titan piping. Is it safe to do that? If not why? Regards Roger F
HI! I have a small question that I hope someone can help me answer. I want to connect an flow-element made of Hastalloy C22 into a Titan piping. Is it safe to do that? If not why? Regards Roger F
Nov 16, 2004 #2 EdStainless Materials Joined May 20, 2004 Messages 16,376 Location Waukesha WI USA Do you mean titanium? What is the fluid that you are handling? If there is chance for galvanic corrosion you should not do it. = = = = = = = = = = = = = = = = = = = = Corrosion never sleeps, but it can be managed. http://www.trenttube.com/Trent/tech_form.htm Upvote 0 Downvote
Do you mean titanium? What is the fluid that you are handling? If there is chance for galvanic corrosion you should not do it. = = = = = = = = = = = = = = = = = = = = Corrosion never sleeps, but it can be managed. http://www.trenttube.com/Trent/tech_form.htm
Nov 16, 2004 Thread starter #3 RogerF Mechanical Joined Oct 7, 2002 Messages 11 Location NO HI Yes i ment Titanium. The fluid is Seawater with 300 ppm Hyprocloritt Will this information help you to say yes og no? Roger Upvote 0 Downvote
HI Yes i ment Titanium. The fluid is Seawater with 300 ppm Hyprocloritt Will this information help you to say yes og no? Roger
Nov 17, 2004 #4 metengr Materials Joined Oct 2, 2003 Messages 15,478 Location US How do you intend to attach the Hastelloy C-22 flow element to the Ti piping? If it can be attached by mechanical means to the piping, a nonmetalic gasket should be used to prevent direct contact between the Ti and Hastelloy. Upvote 0 Downvote
How do you intend to attach the Hastelloy C-22 flow element to the Ti piping? If it can be attached by mechanical means to the piping, a nonmetalic gasket should be used to prevent direct contact between the Ti and Hastelloy.
Nov 17, 2004 #5 stanweld Materials Joined May 9, 2003 Messages 2,906 Location US Use a a mechanical jointing system. The two materials cannot be fusion welded together without the use of an intermediary metal or metals. Upvote 0 Downvote
Use a a mechanical jointing system. The two materials cannot be fusion welded together without the use of an intermediary metal or metals.