Continue to Site

Eng-Tips is the largest engineering community on the Internet

Intelligent Work Forums for Engineering Professionals

  • Congratulations JAE on being selected by the Eng-Tips community for having the most helpful posts in the forums last week. Way to Go!

Supplemental hardness testing

Status
Not open for further replies.

WE91

Industrial
Nov 29, 2023
13
ASME Section IX

I Have a WPS that is qualified up to 8" but the hardness limit is slightly above client requirement. Would a retest on a 1/2" coupon for hardness testing allow me to maintain my upper limit of 8" when if I combine the PQRs in accordance with QW200.4?
 
Replies continue below

Recommended for you

Yes PWHT is required
 
You should take hardness before and after PWHT.
There may be something wrong with the PWHT.
You've done it?

Regards
 
PWHT is fine hardness readings are well within MRO175, MR0103, and SP0472, but client specs are restrictive.
 
You can increase the PWHT temperature slightly on your supplementary test coupon to accommodate your customer’s hardness requirements; as long as you stay below the lower transformation temperature. This is per ASME Section IX.

The devil is in the details; she also wears prada.
 
I suggest increase the holding time and slower cooling rate of PWHT.