Does anyone have experience with using sulfamic acid to clean C-2000 equipment?

I've found literature for C-276 in 10% sulfamic (0.002 mils/yr) but nothing for C-2000. My main concerns stems from the Copper in C-2000. Our contractor acid cleaners use sulfamic but have a note in their documents: "Sulfamic acid is not an acceptable solvent for use in systems whose materials of construction include copper or copper alloys, because of the possibility of stress corrosion cracking.". Haynes shows C-2000 composition at 1.6%wt Cu. Any concerns with cleaning a C-2000 vessel with sulfamic? Or any recommendations on literature that would help me understand the SCC concerns specific to the copper? Thanks

 
Replies continue below

Recommended for you

That amount of Cu is not an issue. At these levels it is all in solution and SCC from sulfamic is not an problem.

= = = = = = = = = = = = = = = = = = = =
P.E. Metallurgy, Plymouth Tube
 
Thanks EdStainless! This is in line with what I've found elsewhere. In case anyone else has this question in the future; we spoke with a Haynes (manufacturer of C-2000) metallurgist, his response was (paraphrased):

"Copper is a substitutional atom for the Nickel so it’s part of the crystal matrix and not present as a precipitate or secondary phase. If anything, I would expect the C-2000 to be slightly more resistant to Sulfamic than C-276."
 
I can confirm EdS's advice, having looked at this issue in depth a couple of years back.

"If you don't have time to do the job right the first time, when are you going to find time to repair it?"
 