1
We are having problems with anolyte for a electrocoating application. The colour of the anolyte (acetic acid) has changed from a normal pale yellow to a dark red/black colour. It is suspected that the 316 stainless steel anodes may be "dissolving" as high concentrations of Cr, Ni and Mo are found in the anolyte solution. A change of voltage has been tested through the anodes recently, could this be the source of the problem? Any other theories on the topic?
 
Replies continue below

Recommended for you

316 stainless, if made anodic at a voltage that puts it in the transpassive region, will dissolve. What voltage is required is a function of the specific solution and it's temerature. Your hypothesis seems quite likely.
 
A good place to look for more information on this topic is the website for Products Finishing magazine, specifically the painting section. I highly recommend the site and the magazine (both available for free)-- articles, clinic, and forum are all very useful.

 