Dear All,
I'm designing a Stainless steel Small high pressure vessel (650 psig Pressure design at 250 oF), with conical shell :Top Dia.8in Id, Btm Dia.2in Id, H=20in , thk= 5/16 in, So We are not able to form this conical shell, my question:
what is the ASME Section VIII Div.1, requirement , if we use a machined or forged conical shell part?

Thanks.
Regards.
 
401laurent, I don't believe any of the rules for cones, including Apx 1-5 and 1-8 make any mention at all of product form. I would not plan on machining it from barstock though.

Regards,

Mike

The problem with sloppy work is that the supply FAR EXCEEDS the demand
 
Cylindrical parts machined from bar are limited to a maximum size of NPS4.

Forgings are not a problem, you they are not limited by size.

Can't you bump this in a break press in two pieces then perform two long-seams?
 
Review UG-6 and UG-14. Limits stated by marty007 can be extended using CC 2156-1.
 
Hi Marty007,
I checked in the beginning your suggestion, by welding two formed pieces ,but the calculated forming strain is = 13.644%,which excced 10%, and per UHA44, its require a heat treatment.

Thanks .
 
401laurent, you might want to take another look at UHA-44(a)(1)(b) & Table UHA-44.

Regards,

Mike

The problem with sloppy work is that the supply FAR EXCEEDS the demand
 
Thanks SnTMan,
indeed when I took a deep look to UHA-44(a)(1)(b) & Table UHA-44, and regarding grade material & my temperature design, it doesn't take a heat treatment.

Regards.
 