According to a senior design eng of our firm, the correct material for this vessel (design temp= 100/-128 °C) is SA240 TP304L.

According to ASME Secc 2D (Metallurgical Phenomena), the only materials which do not show a decrease in the tensile yield nor ductility measured as percent elongation are those listed in tables 1B and 2B from section 2B (non-ferrous materials).

So I conclude that this material (SA240 TP304L) could be used only if impact testing is provided.

I'd like to know what you think about this.

Thanks,
Diego.
 
Impact testing would not be required for this material.
 
Depending of welding procedure. See ASME VIII Div. 1 UHA-51

Regards
rhg
 
rhg;
If the MDMT is -186 deg C or warmer impact testing of this material including HAZ's is exempt (see UHA-51 (d)).
 
How about SA-353? It could be used as low as -320F (about -196 dC), right?
Thanks.
 
zjliang;
Yes, it can but it requires CVN impact testing for MDMT at or warmer than -196 deg C (see UHT-6(a)). For colder metal temperatures, in addition to CVN tests, drop weight testing shall be performed (see UHT-6 (b)).
 
It seems very clear now that I read the UHA-51. Sometimes I feel that you have to know this code by heart to find stuff.

Thanks,
Diego.
 