Can anyone explain why the allowable stresses for F316 are higher than F316L in SA-182? It appears that above 850'F, 316L is not suitable wheras 316 has allowable stress up to 1500'F.Other than the low carbon content in the L grade, I see no difference in the composition.
 
That is it, the carbon. It is an interstitial strengthener that gives higher strength across the temp range.
for comparison look at the numbers for 316H.

= = = = = = = = = = = = = = = = = = = =
Plymouth Tube
 
There is a detail that goes un-spoken these days also.
That is the dual certified 316/316L.
One reason that today's L grade will make straight grade mechanical properties is because of a little bit of N in the alloy.
While the nitrogen is a good strengthener at low temp it does not raise creep strength as much as C would.
This is why you are only allowed to use H grades (with min C) in creep limited applications.

= = = = = = = = = = = = = = = = = = = =
Plymouth Tube
 
Please read the notes at the end of the stress lines. This is why they are there and explain the differences.
Example -
G12 At temperatures above 1000°F, these stress values apply only when the carbon is 0.04% or higher on heat analysis.
 