Hi AlexEss
There are many misconceptions about adhesive bonding. So, everyone knows the surface must be clean. However, many people believe that you need to abrade to "rough the surface" so that the adhesive keys into the roughness. So the common perception id that you clean the surface, grit blast and then clean the debris off. Just as you stated.
Let me provide the correct advice. Firstly, adhesive bonding is a CHEMICAL process that relies on having a clean, chemically active surface to enable the adhesive to react with the oxides and hydroxides on the surface of the metal to generate bond strength. But that is not the full story and I will discuss later. So, clean, blast and clean again is the usual method, but remember that the surface must be reactive, and if you clean it a second time to remove the abrasion products, you will leave a layer of solvent contamination and that will inhibit chemical reaction. So, clean first, grit blast and then BLOW the dust off with clean gas such as dry nitrogen. Solvent cleaning will only contaminate the surface.
Now for the critical step. Please realise that one of the primary causes of bond failure in later service is failure of the interface and that is usually caused by hydration of the metal surface oxides over time. Let us be clear: a failure of the adhesive by fracture is a design issue, but a failure at or near the interface is a processing issue.
Atmospheric moisture is absorbed by the adhesives which are usually polar molecules that attract water, and that water migrates along the interface such that hydrated oxides are formed on the surface of the metal. For example Al2O3 will hydrate to form AL2O3.2H2O. For that reaction to occur, the weak chemical bonds between the adhesive and the oxides formed immediately after abrasion must dissociate and that results in the failure of the interfacial layer, causing adhesion disbonding which is characterised by the absence of fracture of the adhesive with the failure propagation mainly at the surface of the metal.
So, how do we stop this? We treat the metal surface IMMEDIATELY after grit blasting with chemicals that prevent the hydration of the oxide layer in later service. When we implemented this process for aircraft repairs at one aircraft base, we reduced the bond failure rate from 40% to 0.06% over a study period of 17 years, and even then by using adhesive bond failure forensics, we could tell where the technicians took short cuts that caused these failures. There are paers on this at my web site.
Happy to talk further.
Max
Adhesion Associates