Some MT testing was recently performed on some Abrasion Resistant iron castings.
We finish machine the two "sides" of the castings in a surface grinder with coolant, holding the part with a magnetic chuck.
After one side is machined, the part is flipped, and the opposite surface is machined (ground).
Non fluorescent LPT testing by our level II inspector showed absolutely NO indications.
A third party Level II inspector came in and did wet fluorescent MT inspection, and found what he called "chatter" indications on both sides of nearly every part, caused by improper grinding practices.
He decreed the indications relevant, and the parts no good. ( The acceptance criteria are our call )
Attached is a picture showing the "chatter" pattern, and the pole spacing on the mag chuck in the surface grinder.
We are about to begin a few tests for residual magnetism with a tiger stripe pattern like the "chatter", and if any is found, a thorough demagnetization and repeat MT inspection of a few blades by the 3rd party. Also a chemical etch of some kind to see if there hardness etc variations that correspond to the chattter.
** What are your opinions of the similarity of the "chatter" indications and the mag chuck pole spacing ?
thanks,
Dan T
We finish machine the two "sides" of the castings in a surface grinder with coolant, holding the part with a magnetic chuck.
After one side is machined, the part is flipped, and the opposite surface is machined (ground).
Non fluorescent LPT testing by our level II inspector showed absolutely NO indications.
A third party Level II inspector came in and did wet fluorescent MT inspection, and found what he called "chatter" indications on both sides of nearly every part, caused by improper grinding practices.
He decreed the indications relevant, and the parts no good. ( The acceptance criteria are our call )
Attached is a picture showing the "chatter" pattern, and the pole spacing on the mag chuck in the surface grinder.
We are about to begin a few tests for residual magnetism with a tiger stripe pattern like the "chatter", and if any is found, a thorough demagnetization and repeat MT inspection of a few blades by the 3rd party. Also a chemical etch of some kind to see if there hardness etc variations that correspond to the chattter.
** What are your opinions of the similarity of the "chatter" indications and the mag chuck pole spacing ?
thanks,