hello friends

i have received a Mill test certificate of 250 mm round bar grade AISI 4130 75 ksi(PSL 3,P+X) which i need to verify if the material comply all the requirements of API 6A 21st Edition. however in the MTC its mentioned the QTC size as 4"x4"x8".
NOte that the bar i recieved is more than 1000 lbs. so i need to know whether the QTC size in the MTC is correct as per API 6A 21st edition. please advise in detail regarding this topic

6a21st_f3djcb.png


regards
 
API 6A includes requirements for equipment, specific to the type of equipment or component, and dependent on many factors. The bar MTR you have appears to meet the material requirements for some API 6A equipment but not all API 6A equipment. Note that a 4"x4"x8" QTC has a 5" ER. Whether the QTC size meets the API 6A requirements depends on the following:

1. Is the bar heat treated in a continuous furnace?
- if yes, then per 6.4.1 the QTC must part of a full-size bar, and this material would not meet the API 6A material requirements
- if the bar is heat treated in a batch furnace, continue to the next question

2. Is this considered a casting or a forging?
- if this is classified as a casting, then per 6.4.2.3.1, the QTC ER is required to be equal or greater than the part ER
- bar is usually hot worked, and is usually considered a forging for the purposes of 6A material requirements
- if this is classified as a forging, then continue to the next question

3. Is the equipment required to meet PSL 1 or 2?
- if yes, then per 6.4.2.3.2 the QTC ER is not required to exceed 2.5" (but may), and this material would meet the API 6A material requirements
- if no, continue to the next question

4. Is the equipment required to meet PSL 4?
- if yes, then per 6.4.2.3.2 a prolongation (same diameter as production part) or sacrificial production part is required, and this material would not meet the API 6A material requirements
- if no, continue to the next question

5. (Based on previous answers, the equipment is required to meet PSL 3 or 3G) Will this material be used for a body?
- API 6A includes many different component types, including bodies, bonnets, stems, choke beans, valve bore sealing mechanisms, and hangers
- if this material will not be used for a body, then per 6.4.2.3.2 the QTC ER is not required to exceed 5", and this material would meet the API 6A material requirements
- if this material will be used for a body, then continue to the next questions

6. Is the required yield strength of the body 75K or greater and the bar's weight during heat treat greater than 454 kg (1000 lb)?
- note that the required yield strength of the body may be lower than the minimum specified yield strength in the material specification
- it is likely that only the manufacturer (who controls the design) knows the required yield strength of the body
- the meaning/application of the required yield strength clause is not clear and may have divergent interpretations in some cases, such as when the required yield strength from the design calculations is 74.9K and the material specified on the drawing is 75K material
- if either the required yield strength of the body is less than 75K or the bar's weight during heat treat is less than 1000 lb, then per 6.4.2.3.2 the QTC ER is not required to exceed 5", and this material would meet the API 6A material requirements
- if both the required yield strength of the body is 75K or greater and the bar's weight during heat treat is greater than 1000 lb, then continue to the next question

7. Has the exception in 6.4.2.3.2 (which requires specific design documentation and qualification forging testing) been invoked by the manufacturer?
- if the exception has been invoked by the manufacturer (and the requirements for the exception met), then per 6.4.2.3.2 the QTC ER is not required to exceed 5", and this material would meet the API 6A material requirements
- if the exception has not been invoked by the manufacturer, then per 6.4.2.3.2 the QTC ER is required to match or exceed the part ER up to 250 mm (10 in.), and this material would not meet the API 6A material requirements
 
Dear jmec87

firstly many thanks for taking valuable time and responding to this thread. Kindly note that the subjected round bar is 1.heat treated in a batch furnace
2.bar is forged and have the hot work ratio 11.0 as specified in the MTC
3. Supplier have given a confirmity statement for the bar as "API 6A 75K,PSL 3,P+X & NACE MR0175-03
4.The material is to be used for PQR qualification- butt weld pipe of thickness 35 mm (GTAW root,SMAW-hot & cap)as per 6A 21st edition and hence to be used for the manufacture of 6A body as well
5. the bar weight mentioned in the MTC is 14950 kg which is greater than 1000 lbs
6.All mechanical, chemical ,grain size, charpy impact value(both longitudinal & transverse), heat treatment (normalising, austentization/quenching, tempering) parameters were satisying as per API 6A 21st edition

However i m getting blocked at the QTC size which is given as 4" x 4" x 8"(5 ER). does this also meet the requirement as stated by you in your reply? i am really looking forward for your response

Thanks & regards
 
For a PQR, this material is probably fine. See API 6A 7.3.4.

If you are making a body from this material, then you need to answer questions 3 - 7 above to determine your answer.
 