Continue to Site

Eng-Tips is the largest engineering community on the Internet

Intelligent Work Forums for Engineering Professionals

  • Congratulations waross on being selected by the Eng-Tips community for having the most helpful posts in the forums last week. Way to Go!

QPQ vs. Nitrotec (Gas Nitrocarburizing) 1

Status
Not open for further replies.

toes112

Mechanical
May 23, 2006
9
Besides the environmental differences, is there really any difference to the end product between these 2 surface treatment processes? Hardness, Aesthetics, Durability, Part Deformation would be key characteristics.
 
Replies continue below

Recommended for you

I think where you stated QPQ you meant salt bath ferritic nitrocarburizing (FNC). QPQ is a three-stage process that starts with the salt bath FNC, then has a mechanical polishing step, then a final immersion into another salt bath to oxidize the surface. QPQ has better corrosion resistance and lower roughness than gas FNC, and QPQ is black instead of silver/gray. Both treatments improve the surface hardness of ferrous metals. If your application requires the use of a lubricant, then the wear performance of these two treatments may differ. Otherwise, likely they will behave similarly.
 
In vision applications the QPQ will provide a less reflective flat black background enabling better image definition.
 
Gas nitriding can develop much deeper cases but the risk of spalling of the hardened layer increases with case depth.
 