Again, read the Code which includes me, for 2016 Edition of B31.1, the 0.15%C is based on below
132.3.2 The postweld heat treatment exemptions
of Table 132.2 may be based on the actual chemical composition
as determined by a ladle or product analysis
in accordance with the material specification in lieu of
the specified or maximum specified chemical composition
limits.
For carbon steel P-No 1 in Table 132.2
A preheat of 200°F (95°C) is applied
prior to welding on any nominal material
thickness >1 in. (25 mm)
Multiple layer welds are used when the
nominal material thickness >3⁄16 in.
(5 mm)
See Note (6)
Apparently, when I copied the information it was for P-No 5A and not P-No 1.
My error, so there is no 0.15%C limit for P-No 1 BM.
The above would apply for P-No 5A for information.