Does anyone have a reference or source of information on the density and specific heat of 302 stainless steel? I am particularly interested in any variation on these properties with Cr and Ni content, within specified range for 302 stainless. Thanks.
 
Dear Mr. jmiller68
Mr. butelja just gave you the right place to search, you can find below detailed specifications of what you need from the same place


Regards

Eng. Hamid S. Al-Baghdady
Metallurist


Allegheny Ludlum Stainless Steel Chromium-Nickel Type 302, 0% Cold Rolled (UNS S30200)
Printer friendly version

Subcategory: Metal; Stainless Steel; T 300 Series Stainless Steel

Key Words: Plate, sheet, and strip specs: ASTM A 240; ASME SA-240

Component Wt. %


C Max 0.15
Cr 17 - 19
Fe 72
Component Wt. %


Mn Max 2
N Max 0.1
Ni 8 - 10
Component Wt. %


P Max 0.045
S Max 0.03
Si Max 0.75


Material Notes:
Iron content above calculated as balance.

This alloy is one of the most familiar and most frequently used alloy in the stainless steel family. It may be best used in applications where the following properties are important: resistance to corrosion, prevention of product contamination, resistance to oxidation, ease of fabrication, excellent formability, beauty of appearance, ease of cleaning, high strength with low weight, good strength and toughness at cryogenic temperatures, and readily availability of a wide range of product forms. Food and beverage, sanitary, cryogenic, and pressure-containing applications are examples. Type 302 is preferred over type 304 for temper rolled products since the higher carbon permits meeting of yield and tensile strength requirements while maintaining a higher level of ductility.

Min/max tensile and hardness properties below as requires by ASTM A 240 and ASME SA-240.

Information provided by Allegheny Ludlum Corporation.

Click here to view available vendors for this material.

Physical Properties Metric English Comments


Density 7.9 g/cc 0.285 lb/in³

Mechanical Properties


Hardness, Rockwell B 92 92
Tensile Strength, Ultimate 655 MPa 95000 psi
Tensile Strength, Yield 290 MPa 42100 psi
Elongation @ break 60 % 60 %
Modulus of Elasticity 200 GPa 29000 ksi in tension
Charpy Impact 200 J 148 ft-lb at 23°C

Electrical Properties


Electrical Resistivity 0.000072 ohm-cm 0.000072 ohm-cm
Magnetic Permeability 1.004 1.004 0% cold work
Magnetic Permeability 3.2 3.2 at 50% cold work

Thermal Properties


CTE, linear 20°C 16.6 µm/m-°C 9.22 µin/in-°F Range 20° - 100°C
CTE, linear 500°C 19.8 µm/m-°C 11 µin/in-°F Range 20°- 870°C
Heat Capacity 0.5 J/g-°C 0.12 BTU/lb-°F
Thermal Conductivity 16.3 W/m-K 113 BTU-in/hr-ft²-°F at 100°C; 21.4 W/m*K at 500°C
Melting Point Max 1420 °C Max 2590 °F Liquidus
Solidus 1400 °C 2550 °F
Liquidus 1420 °C 2590 °F
 