Hi Folks,

I am currently liasing with a supplier on the manufacture of a small (25mm X 25mm X 1.5mm)316L stainless steel component.

The component has a Pierce & extrude slot feature which extrudes through 1.8mm (material thickness 1.5mm). Component is cold-worked.

The supplier is currently annealing (for stress relief of the cold working process), then deburring.

Basically my question, is it common to anneal then deburr? If it was me doing this i would deburr then anneal.

It probably does not make much difference in this case, however i have doubts over the competence of this particular supplier hence why i am scrutinising everything they are doing.

All replies welcome.

Gareth
 
Can you describe the annealing process, before we understand the sequence of annealing.

I'm just one step away from being rich, all I need now is money.
( read somewhere on the internet)
 
Yes, slitting before anneal can give you a better edge quality (less burr). However, in your case, the width is only 25mm, the supplier probably rolled a much wider master coil, after annealing, then slitted to 10+ strands. It is less convenient to do slitting first then annealing multiple strands.
 
arun, Annealing is being done at 1100°C for 5-8 mins
 
1100C is more than stress relief, the material will get recrystallization and softened.
The other potential benefit to follow anneal first, then slitting, deburring is to get rid of pull under width issue which could occur during the strand annealing.
 
Either way works.
There is no stress relief of SS, you either anneal or you don't.
If you deburred the 'hard' part you would be less likely to deform the part and you may be able to used a process like vibratory abrasive deburr.
If you anneal first then you may get nicer blending of the edges and a better overall look, and maybe a chemical assisted deburr would work nicely.

= = = = = = = = = = = = = = = = = = = =
Plymouth Tube
 
Ed,
We found stress relieving was not effective for austenitic SS at <1000F, while martensitic and ferritic SS responded better. This seemed to be related to dislocation movement. It is off the topic, but could you know the reason(s)? -Thanks!
 