Hello guys,
I am looking for post weld heat treatment process for Alum 6061 T6 aluminum weldment. I am talking about sizes of street light poles.

[ul]
[li]Procedure[/li]
[li]Temperature requirements[/li]
[li]Holding temperature[/li]
[li]Equipement needed[/li]
[li]Any quenching?[/li]
[li][/li]
[/ul]

I am intending to bring the temper in the HAZ zone back to T6 after this heat treatment.

Any input is appreciated.
 
Replies continue below

Recommended for you

Is the welding filler metal capable of achieving the strength of the 6061-T6?
 
4043 is not capable of meeting 6061-T6. So give up the idea of PWHT. You will simply need to size the materials/weld thickness to reflect the lower strength welds.
 
Thanks for your comments. I did read a little about this.

In the above link from ESAB it states that we need to use filler 4643 in case we are performing PWHT.
Now, I don't know what other changes should be involved in terms of welding equipment etc.
Also, this link says base material as ALUM 6061 T6, but in my case I am welding 6061 T6 extrusion to ALUM 356 casting. Not sure my case is different from what ESAB saying. I will also email their technical support & see what they have to say.

Further coming back to my original question, I believe (I could be wrong) that there is no liquid quenching involved in this PWHT. Just air cooling after 6hrs of holding at 360 deg F is sufficient. Any one know more information about this. or any study material/ resource would be appreciated.