Continue to Site

Eng-Tips is the largest engineering community on the Internet

Intelligent Work Forums for Engineering Professionals

  • Congratulations waross on being selected by the Eng-Tips community for having the most helpful posts in the forums last week. Way to Go!

Pittings in pinion ---- Attn :carburize ( materials)

Status
Not open for further replies.

rkarthik

Mechanical
Dec 16, 2002
19
Thanks for the info.
Actually i wanted to know about pittings forming exactly on the pitch line of the pinion.Is there any relation with the material hardness. I have seen pinions where only in a very few tooth the pittings have been formed and not on all the tooth.
 
Replies continue below

Recommended for you

Pitting usually starts on the pitch line and then spreads to other areas. There are small geometrical differences even in the most accurate gears which means that some teeth (or some areas of some teeth) are slightly more heavily loaded than others and these will be the teeth which pit first.
If I understood your application correctly - on open girth gear and pinions - the geometrical differences can be very large and it is not unusual to see some teeth with no damage and others with pits.
Hardness is a direct factor in the resistance to pitting and if there were large differences between the hardness of the teeth in one area compared to another this could produce the same effect but my observations would indicate that this is less likely than geometric effects causing the pitting to occur in some areas before it appears in others.
 
Status