athomas236
Mechanical
For those of you that have an interest in P91, you may be interested in the following:
On 31 Oct 06 there was a failure in the main steam pipe at Huadian Datong Power Station in China. The failure occurred after the unit had been under going commissioning for a period of 6 weeks. The failure resulted in deaths and other injuries.
Main steam conditions: 2538psig and 1006F
Material: ASTM A335 P91 - 18inch, 1.693 ins thick (seamless)
Rupture was 35 inches long by 1.5 to 2 ins wide and 86 ins from nearest weld.
History of pipe material is still under investigation but preliminary reports suggest the pipe was counterfeit, that is made in China but marked as made in USA.
The Chinese goverment is conducting a formal investigation since pipe is reported to have been used in other plants in China. The use of Chinese made pipe for such critical applications has been banned.
It is thought that some suppliers in the US have placed orders with the mill producing this pipe.
I only learned about this 29 Jan 07 but if anyone has more upto date information, then please advise.
athomas236
On 31 Oct 06 there was a failure in the main steam pipe at Huadian Datong Power Station in China. The failure occurred after the unit had been under going commissioning for a period of 6 weeks. The failure resulted in deaths and other injuries.
Main steam conditions: 2538psig and 1006F
Material: ASTM A335 P91 - 18inch, 1.693 ins thick (seamless)
Rupture was 35 inches long by 1.5 to 2 ins wide and 86 ins from nearest weld.
History of pipe material is still under investigation but preliminary reports suggest the pipe was counterfeit, that is made in China but marked as made in USA.
The Chinese goverment is conducting a formal investigation since pipe is reported to have been used in other plants in China. The use of Chinese made pipe for such critical applications has been banned.
It is thought that some suppliers in the US have placed orders with the mill producing this pipe.
I only learned about this 29 Jan 07 but if anyone has more upto date information, then please advise.
athomas236