For a dissimilar metal weld (DMW) joint to Grade 91, I would use a transition piece of Incoloy 800/800H between the Grade 91 and 316ss. The linear coefficient expansion differences between Grade 91 and 316ss are too large, and will cause cracking problems from thermal/mechanical loads in service.
 
Agree with metengr. We have used this method to preclude cracking of former direct P91 to 316 welds with great success. Original welds failed within 5 startup cycles.
 