Tek-Tips is the largest IT community on the Internet today!

Members share and learn making Tek-Tips Forums the best source of peer-reviewed technical information on the Internet!

  • Congratulations cowski on being selected by the Eng-Tips community for having the most helpful posts in the forums last week. Way to Go!

Nut Steel ISO898 1

Status
Not open for further replies.

wannadie

Mechanical
Joined
Mar 10, 2003
Messages
7
Location
GB
What are the differences between ISO 898-1 grade 8.8 bolt steel and ISO 898-2 grade 8 nut steel?
 
ISO 898-1 & 898-2 do not specify an exact grade of steel. Rather, they define the mechanical property requirements, the allowable range of chemical composition, and whether or not the fasteners must be quenched and tempered. For 898-1, Property Class 8.8, the allowable composition is as follows:

C = 0.25-0.55
P = 0.035 max
S = 0.035 max
B = 0.003 max

The C range is allowed to be 0.15-0.40 if alloying elements such as Mn, B, or Cr are used. The minimum tempering temperature is 425 C.

For 898-2, Property Class 8, the allowable composition is as follows:

C = 0.58 max
Mn = 0.25 min
P = 0.060 max
S = 0.150 max

For sizes below M16, the nuts do not need to be quenched and tempered.
 