Tek-Tips is the largest IT community on the Internet today!

Members share and learn making Tek-Tips Forums the best source of peer-reviewed technical information on the Internet!

  • Congratulations TugboatEng on being selected by the Eng-Tips community for having the most helpful posts in the forums last week. Way to Go!

Nut Splitter Tool, H11? H13? Tool Steel, Good Material? 1

Status
Not open for further replies.

PressEquip

Civil/Environmental
Joined
Oct 26, 2009
Messages
35
Location
CA
Requesting feedback on tool steel material recommendation for nut splitter wedge. Used to split seized nuts, typically A-194 2H [Nuts have max hardness of 38 HRC (327 Brinell)], nut batches are proof load tested based on proof stress of 175 ksi.

In the past, the trades men at the company decided upon M2 tool steel for making the wedges. I developed a heat treating procedure for Austenitize and then quench and temper, required hardness: 62 - 64 HRC. Heat treatment is done in a atmospherically controlled furnace. Hardness testing is done at the end to ensure hardness is in the acceptable range. A hydraulic ram pushes the wedge into the nut to split the nut. The wedge doesn’t get hot, so we could use a low speed tool steel or other suitable grade of steel. But I recently got feedback from the field that the M2 steel wedges aren't holding up well, only splitting a couple nuts and then failing prematurely by brittle fracture.

The tool by hydraulic force puts the wedge in bearing with the seized nut. The wedge is loaded in compression.

I also wonder what material is used in bolt cutter for the jaws. Also the Jaws of Life, used for cutting apart automobiles are the site of accidents, what material is used.

M2 is a high speed tool steel, like for boring tools. Typical Applications include Broaches, Boring Tools, Chasers, Cold Forming Rolls, Cold Heading Inserts, Drills, End Mills, Form Tools, Hobs, Lathe and Planer Tools, Punches, Milling Cutters, Taps, Reamers, and Saws.

Nut splitting isn’t a high speed activity, the wedge probably won’t heat up.

It might make sense to consider changing materials to a tool steel that is good for heavy duty compression tool like H11 or H13, which is also used to make shear blades (similar to how the wedge splits the nut). There are some other grades of tool steel that are also used to make shear blades: D2, A6, A2 DCF, L6, S5. It might be worth considering those grades of steel as well.

Below from the internet

H11 is a chromium-based steel alloy from the “H” family of steels according to the AISI classification system. H11 is one of the most commonly used alloys from this group, thanks to the outstanding impact toughness. Other steels from this group, such as the H13 have more vanadium, which gives better wear resistance and temper resistance, but worse impact toughness. H11 is also used for hot tooling applications thanks to its excellent resistance to cracking, including thermal fatigue cracking, gross cracking and thermal shock during water cooling. These include hot punches, die casting dies, forging dies, hot shear blades, hot gripper dies, and extrusion tooling. Like most steels with high toughness and low carbon content, Steel H11 can be used for producing hot-work steels with the water-cooling method. H11 has minimal distortion during deep-hardening and air-hardening thanks to the balanced alloy content. H11 can also be hardened with an air quenching method.

H13 is a 5% chromium hot work tool steel designed for applications that require extreme toughness combined with good red-hardness. H13 will allow an extra margin of safety in tools subject to heavy hammer blows, and those containing deep recesses or sharp corners. Although H13 was designed as a hot work steel, it has solved many cold work applications where extra toughness could be gained with some sacrifice of wear resistance.
Typical Applications: Aluminum Extrusion Dies, Die Casting Dies, Heavy Duty Compression Tools, Forming Punches, Hot Forging Dies, Shear Blades, Plastic Mold Dies, and Bolt Dies.

D2 is an air-hardening, high carbon, high chromium tool steel with extremely high wear resisting properties. It is a very deep hardening steel and will be practically free from size change after proper treatment. The high percentage of chromium gives it mild corrosion resisting properties in the hardened condition.
Typical Applications: Blanking Dies, Forming Dies, Coining Dies, Slitting Cutters, Heading Tools, Long Punches, Forming Rolls, Edging Rolls, Master Tools, Beading Rolls, Intricate Punches, Extrusion Dies, Drawing Dies

A6 is an air-hardening, non-deforming tool steel that combines the deep hardening characteristics of air-hardening steels with the simplicity of low temperature heat treatment possible in many of the oil-hardening grades.
Typical Applications: Blanking Dies, Precision Tools, Forming Dies, Coining Dies, Master Hubs, Shear Blades, Plastic Molds, Spindles, Mandrels, Heavy Duty Punches.

A2 DCF Tool Steel is an air-hardening grade of steel that contains 5% chromium. A2 is noted for its good toughness and excellent dimensional stability in heat treatment. Replaces the oil hardening (O1 type) when safer hardening, less distortion and increased wear-resistance are required. These characteristics make it a versatile tool steel that combines good performance and price. A2 Steel falls between oil-hardening and D2 high-carbon, high chromium tool steels.
Typical Applications: Large Blanking Dies, Thread Roller Dies, Long Punches, Rolls, Master Hubs, Trimming Dies, Forming Dies, Precision Tools, Gauges, Coining Dies, Extrusion Dies, Mandrels, Shear Blades and Slitters.

L6 is a tough, oil-hardening tool steel possessing a fine-grained structure and desirable shock resistance. L6 is also associated with high strength and good non-deforming characteristics.
Typical Applications: Forming Rolls, Spindles, Punches, Trim Dies, Blanking Dies, Embossing Dies, Forming Dies, and Shear Blades.

S5 is an oil-hardening silicon-manganese steel of medium carbon content especially adapted for punches, shear blades, chisels, and other shock resisting applications. S5 is therefore applicable where the properties of silicon-manganese steels are desired in combination with well-known advantages of oil-hardening steels. A reduced tendency to distort or crack in heat treatment is accordingly combined with high toughness in S5.

Do you think we should consider changing from M2 tool steel to another grade of steel for this application? If so, what grade of tool steel and what harness range to aim for?

Thanks in advance for the feedback!




A Fan of EngTips, share the knowledge
 
M2 should be fine, are they hardening the tip only, like a chisel, only the tip i harden to 60 HRc, don't through harden the entire tool, that is why it will fail. the rest of the tool needs to be tempered , or through harden the entire tool to 40 HRc, then induction harden the tip to 60-65 Hrc
 
Thanks mfgenggear for the response!

The parts are small, made from 1.38" OD to 1.588" OD annealed round bar into a triangular shape (chisel). We make a couples different sizes of wedges.

They are double tempered, then hardness tested, if too hard (above 64 HRC) then a third temper is done

This is what my current heat treating procedure states for tempering: Double temper is mandatory, three tempers are sometimes preferred (for large cross sections, over 2”). First temper heat to 1050°F ± 25°F, soak for 2 hours per inch of thickness. Air cool to ambient between tempers. For the second and potentially third temper, the tempering temperature is at the discretion of the heat treating company. This discretion is to enable the heat treating company to adjust the tempering temperature if required with the intention to achieve final hardness testing results within the acceptable range.

mfgenggear, what are your thoughts on the above?





A Fan of EngTips, share the knowledge
 
I think you are missing mfgenggear's suggestion: You don't need nor want the entire tool anywhere near your 64 HRC, just the tip.
 
mfgenggear, thanks for the link to the data sheet!

From M2 tool steel data sheets, striving for 62 to 64 HRC seems to be the sweet spot for trying to optimize both high hardness and high impact strength.

With how we use the parts, they fail in brittle fracture, not yielding in compression.

How low in hardness do you think I can go and the tool still be hard enough to split the sieved nuts (nuts spec. requires max hardness of 38 HRC)?

Do you think I should consider changing to a different grade of tool steel?

A Fan of EngTips, share the knowledge
 
BiPolarMoment, with the parts being relatively small, it makes it more challenging to case harden. Like mfgenggear suggested, through harden to 40 HRC and then induction harden the case so the tips are 60-65 HRC. That is interesting and worth considering; lots of steps and might not be very efficient/optimal. I'm assuming the case will need to be tempered. The literature I've read on M2 tool steel doesn't mention case hardening; might be blazing a new trail.

Also, I'm not sure if the heat treater can do induction hardening of the case in a controlled atmosphere so decarbonization is prevented.

A Fan of EngTips, share the knowledge
 
It didn't sound like your parts were all that small based upon your only mention of the starting OD. What is small (presumably) is the edge that is doing the 'splitting'--which is why induction hardening is appealing in the first place. You can heat up that area quickly without heating up the rest of the part; it's used all the time on things like saw blade teeth to increase hardness without making the rest of the tool brittle.
 
Thanks BiPolarMoment for the information and feedback!

A Fan of EngTips, share the knowledge
 
If you don't want to try localized hardening ...
For a test you could try tempering some like they do some knife blades.
You harden the whole part to 62 HRC.
Now there are two options.
1. The cover the tip (maybe 1/3 of the way down) with wet clay.
Then place in the furnace with the temper temperature set for 40-45 HRC.
You will have to experiment with the time, once the clay dries out the tip will begin to temper more.
You may have to do a few short tempers to get this.
2. Fill a small steel box with sand and wet it well.
Place the tip of the wedge into the sand (again about 1/3 of the way).
Put into temper to 45 HRC
Them moisture in sand will keep the tip from softening too quickly.
I have used both of these with knife blades.

= = = = = = = = = = = = = = = = = = = =
P.E. Metallurgy, consulting work welcomed
 
Thanks EdStainless for the feedback! Interesting how you heat treat the knives you make!

My plan is to change material for the next batch we make. I'm still evaluating the options.

A Fan of EngTips, share the knowledge
 
I would go with H13. temper at lower temperatures 1000F to get a higher hardness (>50HRC) still with a good toughness. double temper at a bit lower temp.

A star to ED, unique method!
 
look at the tempering section of the data sheet for M2, to retain hardness and obtain full toughness, triple temper
also an other old technique for chisels was after quench draw the shank back with an acetylene torch . thus it will mushroom slightly but not crack.
check out the procedure for manufacturing chisels.
 