Weigh parts
Reduce melt temp to minimum that will pack the mould. Increase mould temperature if necessary to obtain a good part at the minimum melt temp
Increase injection pressure until machine max or just short of flash
Weigh new parts
Increase injection hold time
Weigh parts
Keep increasing injection hold time untill parts do not increase in weight.
Physically cut parts to inspect for voids
If voids present, increase gate/runner size
Weigh parts
Repeate process above.
Increase gate/runner etc untill no voids present.
Use final weight as QC test.
Clear material might help, but colours can change moulding characteristics, including tendency to form voids, so once good solid mouldings are achieved clear, mould colours, then test as above
Regards
pat