I'm reading a topic about stainless steel nitriding at high temperatures > 480 C which is mainly caused by gaseous NH3.
I read nothing about N2, does N2 not react with the stainless steel?

thanks in advance
 
Replies continue below

Recommended for you

The lower end of the nitriding temperature range is usually given as 495°. NH3 is in fact used for the nitriding atmosphere, so there definitely is potential. N2 will react with nitride formers, led by Al (the strongest), but also including Cr. I would be concerned about local Cr depletion and loss of corrosion protection, but I have no hard information to pass on about that.

ASM

"Everyone is entitled to their own opinions, but they are not entitled to their own facts."
 
I have ion (plasma) nitrided 304L.
We were doing this at 500-550C (I don't recall exactly).
It can be done at lower temp, such as 360-400C.
At lower temp you don't form Cr nitrides and there is no impact on corrosion resistance.
Look up papers by Swagelok.

= = = = = = = = = = = = = = = = = = = =
P.E. Metallurgy, Plymouth Tube
 