ni625 solid pipe yield strength is normally at 60ksi, if I want to increase it to 65ksi. Is this acceptable for this material. Can i get this 65ksi from stockist or do i need to get it customised for the process.

regards
 
Replies continue below

Recommended for you

You would need to either find material in stock that happened to meet your requirement, or go to a mill.
Since the 60ksi material is the low temp anneal (not full solution) I don't know how much margin there is to offer a higher strength.

= = = = = = = = = = = = = = = = = = = =
Plymouth Tube
 
I took it to mean seamless.

= = = = = = = = = = = = = = = = = = = =
Plymouth Tube
 
What are you actually asking: is it to try and get an SMYS increase for design purposes?

Steve Jones
Corrosion Management Consultant


All answers are personal opinions only and are in no way connected with any employer.
 
SJones:- you are right I am looking to increase the design SMYS limit .
 
I see 625 bar above 65ksi yield quite often. It's the result of cold-work with a relatively low temp "stress relief" (e.g. - 1600F). A full solution anneal at higher temps will lower it back down to close to 60ksi yield. Call a mill or distributor and see what they have in stock, I'm sure they will have a heat with yield higher than 65ksi.
 
But will the design specification allow the use of actual mechanical properties as opposed to specified minima?

Steve Jones
Corrosion Management Consultant


All answers are personal opinions only and are in no way connected with any employer.
 
Oh I see. If you need similar corrosion resistance with higher strength (e.g. - double the strength) you could always go with 625+/725.
 