To Rob, Nigel, and SparWeb
The NAS1097 rivet is developed by Douglas aircraft with a reduced countersunk head. The MS20427 rivet is a larger countersunk head which can knife-edge the skin (sheet). MIL HB-5 provide the bearing/shear failure of the joint strength. MIL HB-5H (Latest J) table 8.1.2.2(C) shows the MS20426AD (Fsu 30ksi) ultimate shear strength of the rivet in different sheets.
The thinner the sheet you may have to use (multiply) by the rivet reduction facor (table 8.1.2.1(b).
For example: you have a 0.063" thick sheet, using NAS1097AD5 or MS20426AD5 rivet. You calculate what is the countersunk depth and subtracted from the skin thickness (0.063"

. The hole size for #5 rivet is 0.161/0.166" dia. Countersink dia. for NAS1097 is 100 deg countersink 0.226/0.236" and for MS20426AD5 rivet head dia. 100 deg c'sink 0.267/0.277".
For rivet use Min. csk dia with max hole dia to give you the critical condition. to calculate the remaining thickness at critical condition, t_rem = t_skin-(Max Csk Dia-Min Csk Hole Dia)/2*tan(50).
For NAS1097 head: t_rem =0.027" >0.010 to prevent from Knife-edge (O.K for design)
For MS20426 head: t_rem =0.003" <0.010 to Knife-edge condition (not good for design, fatigue problem)
Using these remaining thickness and calculate your rivet shear strength along with the rivet reduction factor.
Fsu (AD rivet) = 30 ksi, Psu (NAS1097AD5 rivet) = Fsu*PI/4*(Min Hole Dia)^2*RF for 0.025" (from MIL-HB-5 rivet reduction factor 0.925) = 564 lb. Similarly the MS20426AD5 rivet can be calculated for 520 lb (with 0.86 reduction factor estimated). Thsi is how the MIL HB-5 joint allowables are established from test and reduction tables are developed. This is just the rivet shear capability.
You need to calculate the rivet bearing strenth. Which is based on the material ultimate bearing strenth at Min. 2xDia. for the least material property (eg. 2024T3 compare to 7075-T6 AL). Pbru = Fbru_2D*t*Min. Hole Dia.
Let say the 2024-T3 clad Fbru (2D) = 125 ksi and 7075-T6 clad sheet Fbru (2D) = 146 ksi.
If your skin is 2024-T3, then Pbru = 1268 lb and for 7075-T6 Pbru = 1481 lb. You are allowed to use effective hole dia. for your bearing strength accounted for the csk larger area.
The failure of the joint is in rivet shear and not bearing failure. That is why NAS1097AD5 rivet joint failure load on 2024-T3 skin is 564 to 570 lb. and MS20426AD5 rivet is 520/523 lb.
Hence when you design the structure or repair you make sure you are using the min. joint allowable.
If you need any help let me know.
Good luck.
Richard Chwa