Hi All
Based on the FEED report the properties of produced water is Chloride 1,43,000 ppm and H2S 1000ppm. But material selected is CS with 6mm CA and Valve trim is SS316. I want to know is it possible to use SS trim with out any coating for this chloride content and for the pipe also no internal coating is mentioned for CS material.

 
Could you edit your post and fix the number? Is it 1.43 million ppm or 143 thousand ppm? Kind of a big difference since I don't think that 1.43 million ppm (or 1.43 kg/L = 1.43 kg/kg) is possible. If you'll fix yours I'll delete mine and we can have a conversation.

[bold]David Simpson, PE[/bold]
MuleShoe Engineering

In questions of science, the authority of a thousand is not worth the humble reasoning of a single individual. Galileo Galilei, Italian Physicist
 
Hi
Its 143 thousand ppm.Please find the attached file for more details.

 
You may have pressed the submit button too quick - no file attached? Also state normal and max stream temperature and any info on dissolved O2.
 
A water analysis would be useful. The parameters I'm usually most interested in is pH, TDS, and sodium. 143 gm/L of Cl- is about the same as we see when Barnett wells are drilled into the Ellenburger. Nothing wrong with using carbon steel with that. The H2S could be a problem, but if the pH is high enough then is more a health hazard than a real corrosion issue. People tend to use NACE trim for anything with H2S in it, and I don't have a problem with it. The NACE elastomers are pretty bullet proof and the spec is very specific about not allowing any "yellow metal".


[bold]David Simpson, PE[/bold]
MuleShoe Engineering

In questions of science, the authority of a thousand is not worth the humble reasoning of a single individual. Galileo Galilei, Italian Physicist
 
If you are wishing for the valve to comply with ISO 15156, then that trim material selection will not meet such a wish.

Steve Jones
Corrosion Management Consultant


All answers are personal opinions only and are in no way connected with any employer.
 
For the pipe materials ,I think the best way is have a simple test for the medium . For instance ,put a sample bar into the medium , and observe it's appearance changes .