I get confused.
When looking in manufacturers catalogues I find pipes/tubes having both WPxxx and TPxxx designations. On the other hand, I am also finding fittings with both designations. My understanding has so far been that TPxxx refers to tubes/pipes only and that WPxxx refers to the fittings.

Can someone please clarify this for me.

PS. I am European and therefor not completely used to ASME/ASTM specs.
 
Replies continue below

Recommended for you

LSThill,

Thanks for the dimension spreadsheet!
Very nice work.

**********************
"Pumping accounts for 20% of the world’s energy used by electric motors and 25-50% of the total electrical energy usage in certain industrial facilities."-DOE statistic (Note: Make that 99% for pipeline companies)
 
Thanks LSThill, great spreadsheet. It will undoubtedly come in handy.

Unfortunately it didn't answer my question. I think I perhaps were a bit unclear. It is the material designation that I have a problem with.
- Can a tube/pipe be of WP316L (example) or is always TP316L?
- And vice versa, can a fitting be of TP316L or is it always WP316L?
 
STALguy,

I think you are crossing up two ASTM standards.

ASTM A312 is for pipe. The grades of material are prefixed by TP.

ASTM A403 is for wrought fittings. The grades of material are prefixed by WP (other prefixes exist, see the standard).

An A312 TP316 pipe will typically be used in conjunction with fittings from A403 WP316 (wrought), A351 CF8M (cast), and/or A182 F316 (forged).
 
Since STALguy said he was looking at manufacturer's catalogs, it might be that the manufacturer is trying to be helpful and saying for pipe TPxxx, you need fittings WPyyyy.

Patricia Lougheed

Please see FAQ731-376: Eng-Tips.com Forum Policies for tips on how to make the best use of the Eng-Tips Forums.
 
Thanks Steven,
That was exactly what I wanted to know.
Unfortunately I think that there are quite a lot of non-US manufacturers that confuses these designations. At least judging from their catalouges.
That why I asked, just to be sure. Again, thanks.
 
Can't recall the orginal source, but here's what I remember.

TP = Tubular Product (pipe, tubing)
WP = Wrought Product (tee, elbow, reducer...)
F = Forging (flange, sw fitting....)

So for a 316/316L stainless steel system:

Pipe would be ASTM A312 TP316/316L
Elbow would be ASTM A403 WP316/316L
WN flange would be ASTM A182 F316/316L

Regards,

donf
 