Does stainless ever become magnetized? I am using bearings in a turbine and worry than the 80,000 RPM will magnetize the races. Thanks
 
It depends on the formation of ferrite.
 
It depends on the type of stainless steel being used for races. Austenitic stainless steels (2** and 3**) won't magnetise, but ferritic stainless steels and martensitic stainless steels (groups 4** and 5**) are magnetic. Precipitation hardening stainless steels and duplex stainless steels need to be considered on a individual case by case and at the operating temperature.
 
cold deformation can make 304 types magnetic
 
300 series austentics will magnetize when cold worked, not to the level of ferritic stainlesses, but enough to throw off sensetive magnetic sensors. There are 300 series that cold work faster than others however. Nickel alloys will not magnetize but pure nickel is very magnetic. The addition of significant alloy content makes it nearly completely non-magnetic.
 
What type of SS are you using, most bearings that I have used are 440c ss, very magnetic.
 