His 430 may be martensitic, it depends on the C level.
What is the heat treat condition of the 430 and the C?
What is the heat treat condition of the A286?
For a good weld you really need both of them annealed, but then you don't have strength in your A286.
Using a Ni based filler will get you closer in thermal expansion, 309 is asking for trouble with these alloys.
There are a number of fillers that would work. NiCrFe-6 is common.
= = = = = = = = = = = = = = = = = = = =
Plymouth Tube