Dear Sir,
Duplex stainless steel can easily pass the intergranular corrosion test in ASTM A262 actual E. If the duplex stainless steel has already undergone ASM G48 pitting corrosion test, is intergranular corrosion test required for duplex steel?
Thank you
 
No, you don't do A262 on a duplex.
You do a A923 on duplex to check for detrimental phases.
Similar to a G48, but different.
It requires full cross sections and freshly ground surfaces.
Or low temperature impact toughness.
Don't allow passing based on microstructure.
 
No, you don't do A262 on a duplex.
You do a A923 on duplex to check for detrimental phases.
Similar to a G48, but different.
It requires full cross sections and freshly ground surfaces.
Or low temperature impact toughness.
Don't allow passing based on microstructure.
Thank you. For type approval tests of duplex stainless steel, including chemical composition, mechanical properties, detecting detrimental intermetallic phase according to ASTM 923, pitting corrosion test according to ASTM G48.However, intergranular corrosion according to ASTM A262 is not required. Is it correct?
 