We have some data for twill weave HS carbon in epoxy which shows an increase in compression compression modulus for hot/wet tests.
Over RT/dry in the 2-direction this is about 15% for 90°C/wet (13% for 70°C/wet). In the 1-direction it is an increase of 9.5% at 90°C/wet (9% for 70°C/wet). There is also a small increase of 1.1% for 70°C/dry in the 1-direction.
It is an average of several tests, probably between six and ten (not sure but this was qualification testing).
I would expect compression modulus to go down for hot/wet. There are small reductions in the tensile modulus figures (except for a 5% increase for 70°C/dry).
Does anyone have any idea what could be going on?
Tabular summary:
[tt]
Test Condition E GPa % change
Tensile 0° RT/dry 61.37
70°C/dry 64.37 4.9
70°C/wet 61.63 0.4
90°C/wet 59.29 -3.4
Tensile 90° RT/dry 59.5
70°C/wet 56.07 -5.8
90°C/wet 58.4 -1.8
Compression 0° RT/dry 52.3
70°C/dry 52.93 1.2
70°C/wet 56.85 8.7
90°C/wet 57.29 9.5
Compression 90° RT/dry 48.46
70°C/wet 56.85 17.3
90°C/wet 57.29 18.2
[/tt]
Over RT/dry in the 2-direction this is about 15% for 90°C/wet (13% for 70°C/wet). In the 1-direction it is an increase of 9.5% at 90°C/wet (9% for 70°C/wet). There is also a small increase of 1.1% for 70°C/dry in the 1-direction.
It is an average of several tests, probably between six and ten (not sure but this was qualification testing).
I would expect compression modulus to go down for hot/wet. There are small reductions in the tensile modulus figures (except for a 5% increase for 70°C/dry).
Does anyone have any idea what could be going on?
Tabular summary:
[tt]
Test Condition E GPa % change
Tensile 0° RT/dry 61.37
70°C/dry 64.37 4.9
70°C/wet 61.63 0.4
90°C/wet 59.29 -3.4
Tensile 90° RT/dry 59.5
70°C/wet 56.07 -5.8
90°C/wet 58.4 -1.8
Compression 0° RT/dry 52.3
70°C/dry 52.93 1.2
70°C/wet 56.85 8.7
90°C/wet 57.29 9.5
Compression 90° RT/dry 48.46
70°C/wet 56.85 17.3
90°C/wet 57.29 18.2
[/tt]