Tek-Tips is the largest IT community on the Internet today!

Members share and learn making Tek-Tips Forums the best source of peer-reviewed technical information on the Internet!

  • Congratulations MintJulep on being selected by the Eng-Tips community for having the most helpful posts in the forums last week. Way to Go!

how to turn nitrated-steel cylinder for repair job?

Status
Not open for further replies.

spekkie

Industrial
Joined
Nov 15, 2007
Messages
1
Location
NL
I’m having problems to get a sufficiently smooth surface and trouble with very short toollife.Tried ceramic inserts and diamondtipped.Material to be turned are injection-cylinders used to inject dies with thermoplastics at very high pressure.Size is upto 4000×300×140mm(lenght×outer×inner).These cylinders are nitrates but the inner is worn,and the most of it is to be replaced by a bimetallic piece.
 
Nitrided steel is very hard. The best thing to do is grind, not turn.

Regards,

Cory

Please see FAQ731-376 for tips on how to make the best use of Eng-Tips Fora.
 
agree with corypad. remove the nitrided layer by grinding and then attempt to turn.

Save water Drink Beer
 
I don't think you'll get very good results cuting with a simple lathe bit. Even if it's hard enough to cut the case you'll find that the surface will chip and spall like glass and it will be difficult to get a good finish.

What you need is a grinder attachment for your lathe. It attaches to the toolpost and has an electric grinder wheel.

Don
Kansas City
 
Status