Gentlemen:

Is there a simple, shop based, test that can be used to
distinguish martinsitic SST (400 series) from CRS/Drill Rod?
Hopefully something on the order of grinding wheel sparks,
etc...

Thanks

The more you know, the more you
know you don't know....
 
Dip it in 50% nitric acid. If SS, nothing much will happen. If carbon steel, lots of nasty bubbling and outgassing. Or, dip it a copper sulfate solution. Carbon steel will plate out copper right away, SS will not , or maybe do a little, depending on whether or not it was passivated.
 
Use a magnet to distinguish between 400 series ferritic and martensitic stainless steels and austenitic, 300 series, stainless steels. 400 series are ferromagnetic (strongly attracted to the magnet).

 
Gentlemen:

Thanks for the tips. I will order some CuSO4 and
Nitric Acid for testing. I have a number of bars
which could be 1030, 1045, 416, or 430, based on
receiving records. The sawman cut off the color
codes....

Thanks again...
 
If you have this kind of mix-up with material inventory, do yourself a favor and have a local chemical/metallurgical lab perform a chemical analysis. Chemical analysis costs between $50-$75 a sample, and it is well worth the price. You can't afford to be mixing even various grades of carbon steel in your inventory.
 
I completely agree with metengr. In your case, chemical analysis is a better option.

Rao Yallapragada
 
Sorting can be done with eddy current devices after you have determined carbon and chrome.

 