How to determine G12 if I have E1, E2 and v12?

Fea_pather

Automotive
Joined
Apr 1, 2025
Messages
5
I intend to work with Composites in my simulations. I have a rough idea of the E1, E2 and the v12 properties I wish to use. With this, is it possible to predict the G12 (in-plane shear modulus) that should be defined in the FEA simulation to ABAQUS? Is there a method similar to the isotropic scenario, like G = E / 2 (1+v)???

Note: I intend to use a Plane stress formulation with Lamina material properties.
 
Hello,

For Orthotropic materials, if you know E1, E2, and v12, you generally cannot directly calculate G12 (the in-plane shear modulus) like with isotropic materials. G12 is an independent material property and is not uniquely determined by E1, E2, and v12.

In isotropic linear elastic materials, the way the material deforms under tension (described by E), under shear (described by G), and the lateral contraction/expansion (described by v) are all manifestations of the same underlying, direction-independent material response. The material behaves the same in all directions – tension, compression, shear (not directly through E, but related to E) etc.

So, a complete set of 9 independent properties – E1, E2, E3, G12, G13, G23 and v12, v13 and v23 must be available to fully characterize the material.

Generally, E1 / E2 ratio of 10 – 40 is typical for composites. Generally, E1 / G12 ratio is also between 10 – 40. Typically, G12 to G13 ratio is 1 and G12 to G23 is between 1.5 to 2. Note that, G23 is often lower than G12 and G13. These are generally expected, but I am not sure if they can be applied for all the Composites out there. The above predictions are for unidirectional composites and may not apply for woven composites.

Best Regards,

Vishakh.
 
I suspect Google would find representative values in 2 seconds.
Or see material supplier data sheets.
Or purchase a copy of CMH-17 Volume 2 at sae.org
 