Continue to Site

Eng-Tips is the largest engineering community on the Internet

Intelligent Work Forums for Engineering Professionals

  • Congratulations waross on being selected by the Eng-Tips community for having the most helpful posts in the forums last week. Way to Go!

Hot Dip Galvanizing after PWHT

Status
Not open for further replies.

Mec.tec

Mechanical
Oct 30, 2014
32
We are manufacturing an ACHE in our shop.Material is carbon steel SA 516 Gr 70 and PWHT is required.Client want us to perform Hot dip Galvanizing of box headers external surface only.Please share your views,is there any effect on the mechanical properties of material.Do share an example of similar case if any.
 
Replies continue below

Recommended for you

PWHT after galv will make the galv drip, smoke and run off! Galv tank is about 850°F, and the zinc is molten and 'wet'. PWHT temp is 1100°F and higher.

And a further 850° after 1150° won't hurt anything, IF the header boxes are vented so the heat expansion of the air inside doesn't make them blow up. Galvanizers get pretty sensitive about dipping tightly sealed items into their tanks.
 