Tek-Tips is the largest IT community on the Internet today!

Members share and learn making Tek-Tips Forums the best source of peer-reviewed technical information on the Internet!

  • Congratulations LittleInch on being selected by the Eng-Tips community for having the most helpful posts in the forums last week. Way to Go!

High temp data for SA 387 Gr.22 Cl.2

Status
Not open for further replies.

bagnamento

Nuclear
Joined
Feb 23, 2005
Messages
30
Location
GB
Hi everybody,
I need tensile properties (yield point 0.2% and ultimate tensile strength) data for ASME SA 387 Gr.22 Cl.2 (21/4Cr, 1Mo) steel.
In particular I need experimental data (not ASME II-D design data) for temperatures within 840-1110°F (450-600°C).

Thanks
 
bagnamento;
I found some information that might be of help to you. The elevated temperature mechanical property data is for 2.25% Cr - 1%Mo alloy steel from the following publication "Report on The Elevated Temperature Properties of Chromium-Molybdenum Alloy Steels" compiled by ASTM-ASME Joint Committee on the Effect of Temperature on the Properties of Metals, Tech Pub 151.

The data below pertains to bar. Despite the different product grade, it will at least give you a ballpark estimate on properties - deg F, Ksi

Temp YS (0.2%) UTS
900 F 38.25 63.75
1000 F 35.75 49.75
1100 F 34.25 39.10
 