Continue to Site

Eng-Tips is the largest engineering community on the Internet

Intelligent Work Forums for Engineering Professionals

  • Congratulations KootK on being selected by the Eng-Tips community for having the most helpful posts in the forums last week. Way to Go!

HELP WITH MACHINING & THREADING TUNGSTEN

Status
Not open for further replies.

steveqturn

Mechanical
May 5, 2009
1
I HAVE TO TURN & SCREWCUT 10MM STOCK BAR TO GET AN 8MM THREAD X 9MM LONG HOW CAN I STOP THE CRUMBLING EFFECT I AM GETTING?
 
Replies continue below

Recommended for you

First, let's start with the basic setup that is necessary for turning tungsten: ISO K01 (C-4) carbide tools ground with 15° negative back rake and 0° side rake. Use a chlorinated cutting oil. Typical depth of cut of 1 mm (0.040 inches) should use a speed of 27-32 m/min (90-105 sfm) with a feed rate of 0.18 mm/rev (0.007 inches/rev). The tool should have a large lead angle (side cutting edge angle) of ~ 45°.

Now, is the crumbling occurring when you machine to an external corner? If so, use a support made out of a machinable thermoplastic material such as nylon. Also, use a large chamfer that is machined before the adjacent surface is machined. This chamfer should be sufficiently sized such that there is some metal still left after the turning cut is complete.

source: ASM HANDBOOK Volume 16 Machining

If you don't have this reference, then you really need to purchase it, especially when machining difficult materials like tungsten.
 