Dear Members, please suggest suitable heat treatment of stainless steel 420 grade we have been quenching and tempering it to achieve UTS in excess of 1300 Mom and need % elongation of 8... Results are never stable wrt to elongation while we consistently achieve its required hardness. Thanks in advance
 
Have you tried different austenitizing temps?
Are you sure that you are getting a complete quench?
What is your temper temperature?

Very small changes in C can change HT response a lot.
Typically for 0.35% C I would start with a 1850F aust, it should quench to 53-56 HRC.
Then temper for 2hr at 900F as a starting point.

= = = = = = = = = = = = = = = = = = = =
P.E. Metallurgy, Plymouth Tube
 
Thank you very much Edstainless and metengr for your kind help.
 