heat treating 17-4 ph

Status
Not open for further replies.

brents

Industrial
Dec 15, 2004
34
Hello,

Does anyone know the tempering temperature to heat treat 17-4 ph stainless to 50+ Rc?

I know this is really hard, but water is going through it at about 15,000 psi..

any help would be appreciated,

thanks,
brent
 
Replies continue below

Recommended for you

Rc 50 is in excess of the normal hardness attainable for
17-4.
 
Pressure containing systems should be designed based on tensile and yield strength and not for hardness.
 
brents,

I agree with israelkk: You should not be designing for hardness in a pressurized system. However, I would guess that you are using a conversion chart & desire to have a tensile strength around 250 ksi, based on your desired Rc50. If so, you won't get there with 17-4 PH (according to Mil-Hdbk-5). H900 Condition is 170ksi yield, 190ksi ultimate.

PH13-8Mo will get you a little higher; "Custom 465 Stainless" will go even higher. Need to look at the whole picture, though - ductility might be a different requirement.

Pete
 
Custom 465 is nice stuff, if you can find it, and if you can figure out how to connect to it.

= = = = = = = = = = = = = = = = = = = =