I have a 20 year old PC ABS mix injection molded part that has some pieces broken off it , the part has suffered some UV damage over the years , and is pretty crispy , I have another identical part and am wondering about cutting and gluing pieces from one to the other , I am thinking about using Trichloromethane as a solvent glue. I am wondering if there are more suitable solvents out there for this plastic such as styrene monomer which I have or MEK . Part is opaque . Glue needs to be transparent. This is a decorative trim and has no loads on it after it is put back into place.
B.E.

You are judged not by what you know, but by what you can do.
 
Replies continue below

Recommended for you

MEK will act as a cement, cyanoacrylates glue ABS very well.

H

www.tynevalleyplastics.co.uk

Politicians like to panic, they need activity. It is their substitute for achievement.
 
Thanks Pud,
I have MEK .
Brian.

You are judged not by what you know, but by what you can do.
 
Follow up,
I got the job done, started with MEK then a friend described a clear commercial ABS cement which had ABS plastic, MEK, cyclohexanone, and acetone in it.
This seemed to work quite well, and had some gap filling properties.