Can anybody provide info' with respect to vibration frequency mins/max to initiate fretting corrosion between assembled parts.
 
Replies continue below

Recommended for you

No such things. Fretting corrosion is dependant on much more than just vibration only (material combination, surface roughness, corrodent, surface pressure and so on)
 
There is a very lengthy discussion on fretting in the following reference:

"Electrical Contacts : Fundamentals, Applications and Technology" by Milenko Braunovic´, Valery V. Konchits, and Nikolai K. Myshkin (2006, Taylor and Francis)
ISBN:9781574447279


He talks about a minimum slip amplitude delta for fretting to occur as follows:
delta = 2*(2-nu)*(1+nu)*mu*P*[1-(1-T/<mu*p>)^(2/3) / 8Ea
where a is the diameter of the contact outer radius, E is the Young modulus, nu is Poisson’s ratio, P is
the normal force, mu is the static coefficient of friction between the contact surfaces and T is the
tangential force (T<<mu*P).

Then later he talks about frequency dependence of fretting:

"6.4.4.5 Frequency of Motion
Because fretting is a rate-dependent phenomenon, the contact resistance will be affected by the
frequency of oscillations. The results in Figure 6.17 show the variation of the number of fretting
cycles required to attain a predetermined contact resistance value as a function of the oscillating
frequency. The data shown are for copper vs. copper26 and aluminum vs. tin-plated copper
contact combinations. It is clear that the lower the frequency, the shorter the time to reach a
given level of elevated contact resistance. The observed effect of frequency can be explained in
terms of oxidation factor of fretting. Because oxidation is time dependent, at lower frequencies for a
longer time the contact zone will be exposed by fretting to oxidation as a result of which an increasing number of conducting spots in the contact zone will be closed, thus increasing the contact resistance."


=====================================
Eng-tips forums: The best place on the web for engineering discussions.
 