Hello,

After inspecting of a fired cylindrical vertical heater, two radiant tubes were dented (mechanical damage)at about the medium length of the tubes (photo attache).

From where does this defect result from? How one can confirm such defect is acceptable to remain for several years until the next shutdown? or when tube replacement is necessary?

Fluid: Water
DT; 180 degrees Celsius
DP: 700Kpa
CA: 1.5 mm
Tube: 6"
Tube material: A106 Gr. B

Have a nice work and day

Regards,
 
 https://files.engineering.com/getfile.aspx?folder=b507d28a-2ca9-47e5-889f-11259be012c1&file=New_Microsoft_Word_Document.docx
Is that a dent or a buckle?

Has this come from thermal stress?

Acceptability is quite hard to certain. First see if there are any cracks - dye penetrant maybe?

Can you do some hardness checks on the most deformed bit?

A U/T inspection to get actual thickness?

A more exact dimensional check on what this feature is a sit's difficult to see from the photo

Probably good for the life of the heater, but needs a bit more investigation.

Or just plug it off and remove it or isolate it.

Remember - More details = better answers
Also: If you get a response it's polite to respond to it.
 
You said the fluid circulating inside the tubes is water?

please confirm.

luis
 
RX, UT, DYE PENETRANT, METALOGRAFIC EXAMINATION, HARDNESS MEASUREMENTS, CAN BE USEFUL.

Is there any possibility to have flame impingement?

regards

luis

 
Hello,

Thanks for the input.

Can we skip the metallographic examination in this case?

Flame impingement had less tendency to occur at the respective areas.

Regards,
 