Does anyone know a good reference for obtaining fatigue curves for nitronic 60? I already checked "atlas of fatigue curves" by Howard Boyer.
 
Replies continue below

Recommended for you

I did see actual tabular values for Nitronic 60 based on a brochure that I obtained some time ago (High Performance Alloys, Inc.)

The tabular values were;

Annealed Bar, 1" dia, 37.5 Ksi fatigue limit for 108 cycles

Cold Worked 54.6%, 0.70" dia, 72.5 Ksi for similar cycles

(Fatigue testing on an RR Moore machine).
 