Hi, I've a exudation problem on EPDM compound. it's very curious problem.
I use EPDM of hi-content of ethylene and paraphinic process oil. This row materials are used since 3 years w/o problems and now the oil exudes in both raw and volcanized state.
Several test was made in order to be sure of raw materials quality, and them was ok.
Then, I change Nordel by Keltan 5508, and exudation phenomena disappeared. Other test was reeplace Tolliris oil by other paraphinic oil (of lower flash point) in the original formula and results was no exudation.
So,
Nordel4770 + Tolliris 7200 = exudation
Nordel4770 + Dexil 109 = no exudation
Keltan5508 + Tolliris 7200 = no exudation
Keltan5508 + Dexil 109 = no exudation
If I see the Nordel resultas I could say the problem is the oil, but if I compare the results of Nordel vs Keltan I could say the problem is EPDM too.
The dilemma is: The problem is the EPDM rubber or paraphinic oil or there are other factor?
What might be the causes or conditions for exudation occurs?
Can someone help me or direct me to understand this phenomena?
Formula in phR
Dow Nordel IP4770P 100
Cabot N-550 225
Cabol N-660 20
Total Tolliris 7200 155
OZn 5
Stearic acid 1
Sulfur 1,4
MBTS 0,3
TMTM 1,4
Thanks you in advance
I use EPDM of hi-content of ethylene and paraphinic process oil. This row materials are used since 3 years w/o problems and now the oil exudes in both raw and volcanized state.
Several test was made in order to be sure of raw materials quality, and them was ok.
Then, I change Nordel by Keltan 5508, and exudation phenomena disappeared. Other test was reeplace Tolliris oil by other paraphinic oil (of lower flash point) in the original formula and results was no exudation.
So,
Nordel4770 + Tolliris 7200 = exudation
Nordel4770 + Dexil 109 = no exudation
Keltan5508 + Tolliris 7200 = no exudation
Keltan5508 + Dexil 109 = no exudation
If I see the Nordel resultas I could say the problem is the oil, but if I compare the results of Nordel vs Keltan I could say the problem is EPDM too.
The dilemma is: The problem is the EPDM rubber or paraphinic oil or there are other factor?
What might be the causes or conditions for exudation occurs?
Can someone help me or direct me to understand this phenomena?
Formula in phR
Dow Nordel IP4770P 100
Cabot N-550 225
Cabol N-660 20
Total Tolliris 7200 155
OZn 5
Stearic acid 1
Sulfur 1,4
MBTS 0,3
TMTM 1,4
Thanks you in advance