The above tank is dsigned to API 620 appendix Q , with an inner tank of ASTM A 353 material 31.2 diax 21.2 m height. The outer tank is of 33.2mx 24.2 m height. The inner tank is resting on hard wood block annular foundation , the bottom annular plate of the tank is 9.8 mm and the bottom center field is of 5.0mm, the bottom center field is insulated with 3 layers of cellular glas and the top layer of clean dry sand.The inner tank roof is of suspended aluminium deck from the outer tank roof.
The tank shell insulation consisits of the glass fiber insulation blanket of 150mm thickness and the loose fill expanded perlite. The perlite density assumed for the design is 65kg/m3.
The tank was dried with air and after a period of 3/4 weeks during the rotinr precommissioing checks , it was found that the bottom plates has buckled up and at one location has even buckeled the annular ring and the shell portion has been caved inside at which location the annular ring to the shell welding has also ruptured along the weld sfor aroundf 6inch. lentgh.The side walls has buckled in two locations on the inner tank. However as the inner tank is like an open vessel kept inside the outer tank and any partial vaccum created inside would have buckled in the weakest structure of the roof. There is no deformation noticed on the weakest structures. What other phenomena can cause such a failure. The materials comply to the API specifications and the properties and the PMI are established.
Can there be any influence of the air flow for drying operation for the failures such as a wind loading effct on the inner tank. Higher pressure is ruled out as the tank is equipped with 2 pilot operated safety valves and 2 mannual safety valves, and at no point in time the valves has propped.
The effect of the compressive stress by the insulation blanket and the perlite filling on calculation for the temperature differential of approximately 20 degrees during the drying operation due to the inner wall expansion does not seem to expalin the phenomenon.
Can a limited explosion under the tank bottom possibleas the failure seems to be due to a pressure wave or a very high compressive force on the external surface of thr inner tanks.
I can forward the failure photos if any one can assist in the analysis.
Can any one suggest the points to be checked and the corrective measures.
The tank shell insulation consisits of the glass fiber insulation blanket of 150mm thickness and the loose fill expanded perlite. The perlite density assumed for the design is 65kg/m3.
The tank was dried with air and after a period of 3/4 weeks during the rotinr precommissioing checks , it was found that the bottom plates has buckled up and at one location has even buckeled the annular ring and the shell portion has been caved inside at which location the annular ring to the shell welding has also ruptured along the weld sfor aroundf 6inch. lentgh.The side walls has buckled in two locations on the inner tank. However as the inner tank is like an open vessel kept inside the outer tank and any partial vaccum created inside would have buckled in the weakest structure of the roof. There is no deformation noticed on the weakest structures. What other phenomena can cause such a failure. The materials comply to the API specifications and the properties and the PMI are established.
Can there be any influence of the air flow for drying operation for the failures such as a wind loading effct on the inner tank. Higher pressure is ruled out as the tank is equipped with 2 pilot operated safety valves and 2 mannual safety valves, and at no point in time the valves has propped.
The effect of the compressive stress by the insulation blanket and the perlite filling on calculation for the temperature differential of approximately 20 degrees during the drying operation due to the inner wall expansion does not seem to expalin the phenomenon.
Can a limited explosion under the tank bottom possibleas the failure seems to be due to a pressure wave or a very high compressive force on the external surface of thr inner tanks.
I can forward the failure photos if any one can assist in the analysis.
Can any one suggest the points to be checked and the corrective measures.