13 -- 10g oxalic acid, 100ml H2O
-- Electrolytic at 6V
a) 10-15sec
b) 1min
83 -- 10g CrO3, 100ml H2O
-- Electrolytic at 6V
a) 5 to 60sec -- attacks carbides
88 -- 10ml HNO3, 20ml HCl, 30ml H2O
-- CAUTION can give off NO2 gas, discard solution
before it becomes orange. USE FUME HOOD.
Stronger reaction than Glyceregia.
91 -- 5ml HNO3, 5ml HCl, 1g picric acid, 200ml methanol or ethanol (95%)
-- Same as 1:1 misture of 80(Viella's) & 74(5%HNO3&Methanol)
103-- 20mlHNO3, 4mlHCl, 20ml methanol(99%)
-- Immerse 10-60 sec