Apr 8, 2020 #1 Raza Rauf Mechanical Joined Apr 4, 2020 Messages 9 Location PK Hello Reader, Which electrode to be used for welding grey cast iron with API5L? Moreover, please share the reference for future. Thanks!
Hello Reader, Which electrode to be used for welding grey cast iron with API5L? Moreover, please share the reference for future. Thanks!
Apr 8, 2020 #2 Dhurjati Sen Materials Joined Dec 14, 2017 Messages 1,005 Location IN The non-standard (but effective) practice is to use inconel electrode. DHURJATI SEN Kolkata, India Upvote 0 Downvote
Apr 8, 2020 #3 Tmoose Mechanical Joined Apr 12, 2003 Messages 5,636 Location US Is this a structural weld? Successful cast iron welding requires much more than just a suitable electrode. Have you found information like this ? - https://www.lincolnelectric.com/en-...-detail.aspx?utm_referrer=direct/not+provided Upvote 0 Downvote
Is this a structural weld? Successful cast iron welding requires much more than just a suitable electrode. Have you found information like this ? - https://www.lincolnelectric.com/en-...-detail.aspx?utm_referrer=direct/not+provided
Apr 8, 2020 #4 arunmrao Materials Joined Oct 1, 2000 Messages 4,758 Location IN Any high Nickel(>55%), is usually used. But I have not had much success. Upvote 0 Downvote
Apr 8, 2020 #5 weldstan Materials Joined Jun 24, 2011 Messages 2,806 Location US This is gray iron? Forget about it!! It could be brazed. If ductile iron, a high nickel filler can be used. Upvote 0 Downvote
This is gray iron? Forget about it!! It could be brazed. If ductile iron, a high nickel filler can be used.
Apr 9, 2020 #6 0707 Petroleum Joined Jun 25, 2001 Messages 3,444 Location PT I will try Inconel lm Upvote 0 Downvote
Apr 9, 2020 #7 EdStainless Materials Joined May 20, 2004 Messages 16,363 Location Waukesha WI USA If you have pieces to sacrifice then try welding. Otherwise look into brazing. = = = = = = = = = = = = = = = = = = = = P.E. Metallurgy Upvote 0 Downvote
If you have pieces to sacrifice then try welding. Otherwise look into brazing. = = = = = = = = = = = = = = = = = = = = P.E. Metallurgy
Apr 10, 2020 #8 0707 Petroleum Joined Jun 25, 2001 Messages 3,444 Location PT if it was white cast iron it will be non weldable. luis marques Upvote 0 Downvote
Apr 10, 2020 #9 weldstan Materials Joined Jun 24, 2011 Messages 2,806 Location US Yes. Upvote 0 Downvote